Stress, Strain, and Elastic Behavior

A lesson on how materials respond to loads, from stress and deformation to elastic behavior and material stiffness.

and

: internal force per area

describes the intensity of internal force within a material. Normal acts perpendicular to a section, while shear acts tangent to it. For cross-sectional area AA, internal axial force PP, and internal shear force VV, the average stresses are

σavg=PA,τavg=VA.\sigma_{\text{avg}}=\frac{P}{A},\qquad \tau_{\text{avg}}=\frac{V}{A}.

Both are force divided by area, so their units are pascals: 1 Pa=1 N/m21\,\text{Pa}=1\,\text{N/m}^2. Engineering calculations often use MPa or GPa. Tensile normal is commonly positive, and compressive normal negative.

These expressions give average , not necessarily the at every point. can vary across a section, especially near where loads are applied or in a complex-shaped member. In a straight, uniform bar loaded along its centroid, average normal is approximately uniform away from the load-application regions.

Deformation of a uniform axially loaded bar

For a prismatic bar of length LL, area AA, and elastic modulus EE, an axial force PP produces a length change

δ=PLAE,\delta=\frac{PL}{AE},

provided the bar remains in the linear-elastic range. The relationship captures useful trends: more force or a longer bar produces more deformation; greater area or stiffness produces less. Tension elongates the bar, while compression shortens it.

Source example. A 2 m steel rod has area 200 mm2200\,\text{mm}^2, carries a tensile force of 20 kN, and has E=200 GPaE=200\,\text{GPa}. First convert to compatible units: L=2000 mmL=2000\,\text{mm} and E=200,000 N/mm2E=200{,}000\,\text{N/mm}^2. Its average is

σavg=20,000 N200 mm2=100 N/mm2=100 MPa.\sigma_{\text{avg}}=\frac{20{,}000\,\text{N}}{200\,\text{mm}^2}=100\,\text{N/mm}^2=100\,\text{MPa}.

Then

δ=(20,000)(2000)(200)(200,000) mm=1 mm.\delta=\frac{(20{,}000)(2000)}{(200)(200{,}000)}\,\text{mm}=1\,\text{mm}.

So the rod elongates by about 1 mm under the stated assumptions. If force, area, or material changes along a bar, its total deformation must instead be found by adding or integrating the local contributions; the uniform-bar formula cannot be applied directly to the whole member.

Measuring Deformation with Strain

Strain measures deformation

describes internal force intensity; strain describes the resulting deformation. For a specimen with original length L0L_0 and new length LL, normal (axial) is

εeng=L−L0L0=δL0.\varepsilon_{\text{eng}}=\frac{L-L_0}{L_0}=\frac{\delta}{L_0}.

It is dimensionless because it is a length divided by a length. It may be written as a percentage or in microstrain. The sign indicates whether the length increased or decreased under the chosen convention.

For uniform uniaxial deformation, is

εtrue=ln⁡(LL0).\varepsilon_{\text{true}}=\ln\left(\frac{L}{L_0}\right).

Unlike , it accounts for successive changes in length as deformation proceeds, which matters when deformation is large.

describes a different mode: angular distortion rather than change in length along the bar. Engineering γ\gamma is the change in angle between two lines that were initially perpendicular, measured in radians. For small distortions, it can be approximated by lateral displacement divided by the distance between the sheared faces. This displacement-over-distance approximation is not stated for large distortions.

Thus, axial pairs with length change, while describes angular change. They correspond to different deformation modes, just as describe different directions of internal force.

Elastic Response and Material Stiffness

From recoverable response to failure

A material is elastic when it returns to its original shape after unloading. In the linear-elastic region, is proportional to strain, so uniaxial Hooke’s law applies:

σ=Eε.\sigma=E\varepsilon.

On a –strain diagram, the straight-line portion has slope EE, . A larger EE means less strain for the same in this region.

Two limits describe different ideas. The proportional limit is where and strain stop being proportional; the elastic limit is the greatest from which the material can still fully recover. They need not coincide. Beyond the elastic limit, some deformation remains after unloading: this is .

A typical ductile-material tensile response progresses from linear elasticity through yielding, , and strain hardening. Later, engineering may fall as necking develops, before fracture. Brittle materials generally show little before fracture. This is a typical progression, not a universal curve: the precise response depends on the material and test conditions.

Stiffness in different deformation modes

describe material response in distinct modes:

  • EE measures resistance to axial extension or compression; in uniaxial linear elasticity, σ=Eε\sigma=E\varepsilon.

  • Shear modulus GG measures resistance to shear distortion; in linear elasticity, τ=Gγ\tau=G\gamma.

  • Poisson’s ratio ν\nu is the negative ratio of lateral strain to axial strain under uniaxial loading: ν=−εlat/εaxial\nu=-\varepsilon_{\text{lat}}/\varepsilon_{\text{axial}}. A stretched specimen usually contracts laterally.

  • Bulk modulus KK measures resistance to uniform volume change under pressure. For small volume changes, K=−p/(ΔV/V)K=-p/(\Delta V/V), where pp is the applied pressure magnitude.

For a homogeneous, isotropic, linearly elastic material, only two of the four constants EE, GG, ν\nu, and KK are independent. Useful relations are

G=E2(1+ν),K=E3(1−2ν).G=\frac{E}{2(1+\nu)},\qquad K=\frac{E}{3(1-2\nu)}.

The assumptions matter: anisotropic materials respond differently by direction, so these relationships do not generally apply to them. The constants also describe different kinds of stiffness; for example, EE concerns axial response, while GG concerns shear response.